研究了一种Ti-IF钢在未再结晶铁素体区润滑热轧后、冷轧压下量对IF钢退火后的深冲性能和织构的影响,通过采用非再结晶铁素体区的润滑热轧和随后的冷轧工艺,Ti-IF钢连续退火工艺冷轧板的γ值在73%的冷轧压下星的效果与传统工艺90%冷轧压下量相当,织构分析表明,采用铁素体润滑热轧的热轧板轧制织构中具有较强的{111}//ND组分,当采用73%冷轧压下量和随后的退火工艺可获得最强的{111}//ND再结晶织构,进一步增大冷轧压下量,将减弱〈111〉//ND织构
The effect of cold rolling reduction on deep drawing properties and texturing of IF steel after annealing was studied in a non-recrystallized ferrite zone of a Ti-IF steel. By using non-recrystallized ferrite zone Of the hot rolling and subsequent cold rolling process, Ti-IF steel cold rolled continuous annealing process γ value of 73% of the cold-rolled star effect of the traditional process 90% cold rolling equivalent to the texture analysis It is shown that the {111} // ND component of the hot-rolled sheet with hot-rolled ferritic lubrication has a strong {111} // ND composition. The strongest {111} // ND The recrystallization texture, further increasing the cold rolling reduction, will weaken the <111> // ND texture